Use drying settings for both the exact Bambu filament and the device doing the drying. A temperature from a forced-air oven table is not automatically an AMS setting. The table below follows Bambu’s current AMS guidance for selected common materials.
Bambu AMS drying settings
Scroll horizontally to read the full table. When focused, use the left and right arrow keys.
| Bambu filament | AMS 2 Pro | AMS HT |
|---|---|---|
| PLA Basic / PLA Matte | 45°C, 12 hours | 45°C, 12 hours |
| PETG / PETG-CF | 65°C, 12 hours | 65°C, 12 hours |
| ABS / ASA | 65°C, 12 hours may not fully dry | 80°C, 8 hours |
| PA6-CF / PAHT-CF | 65°C, 12 hours may not fully dry | 85°C, 12 hours |
These are drying settings, not feeding permissions. PA6-CF is excluded from AMS feeding even though it appears in the manufacturer’s drying table. Check the current instructions for spool preparation, rotation and the exact material before starting. Third-party filaments and dryers need their own specifications.
Why different devices have different times
Bambu specifies a maximum drying temperature of 65°C for AMS 2 Pro and 85°C for AMS HT. Some engineering materials need more heat than AMS 2 Pro can provide. Extending a low-temperature cycle is not a verified substitute for the required process.
For PETG HF, the technical sheet separately specifies 65°C for 8 hours in a suitable forced-air drying oven. That does not replace the 12-hour AMS schedule above. Use equipment intended for the selected drying process; Bambu excludes kitchen and microwave ovens in the HF technical sheet.
A practical drying checklist
- Identify the exact grade and whether drying is required before printing.
- Check the spool’s heat rating; install a refill on a suitable spool first.
- Read the device’s rotation/static-drying and power instructions.
- Remove lower-temperature materials when the selected cycle could soften them.
- After drying, protect the spool from moisture with sealed storage and effective desiccant.
Drying, dry storage and diagnosis are different
A sealed box with desiccant helps limit moisture uptake; it is not equivalent to a heated drying cycle for a wet spool. Popping, bubbles and rough extrusion are reasons to check moisture, but those symptoms alone do not prove the dryer or nozzle needs replacement. If drying does not resolve the issue, check the correct profile and the manufacturer’s troubleshooting sequence.
Compare AMS 2 Pro and AMS HT by the materials you actually use. Our AMS comparison covers the systems, while TPU compatibility explains why flexible grades require separate attention.
Frequently asked questions
Does desiccant dry a wet PETG spool as quickly as a dryer?
Do not treat sealed storage with desiccant as a replacement for the manufacturer’s heated drying cycle. Use desiccant to help maintain dry storage after the correct drying process.
Can AMS 2 Pro fully dry every engineering filament?
No. Its maximum drying temperature is 65°C, and Bambu marks several higher-temperature materials as potentially not fully dried by that system. Select a supported device and process for the exact grade.
Can A1 or A1 mini heatbeds be used for the enclosed-printer drying method?
No. Bambu’s heatbed drying instructions require an enclosed printer and exclude the open-frame A1 and A1 mini. Use a suitable dedicated drying method for your filament.
Sources and product checks
Reviewed November 13, 2026. Bambu filament drying recommendations; PETG HF technical data sheet.